摘要:随着 1.6T、3.2T 高速光模块规模化落地,光芯片、VCSEL 阵列、TOSA/ROSA 组件功耗持续抬升,局部热流密度突破传统铜、钨铜、AlN 热沉材料的散热极限,激光器波长漂移、带宽衰减、长期可靠性下降成为行业共性痛点。本文以金刚石 / 铝复合材料(金刚石铝)为核心热扩散材料,面向高速光收发模块开展完整热管理方案开发,从行业需求分析、结构方案设计、热阻理论计算、安装结构设计、精密装配工艺、对比验证实验等环节开展工程化实践。结果表明:采用金刚石铝均热片替代传统铜热沉后,光芯片结温显著降低,器件间温差大幅缩小,热循环可靠性提升,可满足下一代高速光模块高密度封装、低热失配、高带宽稳定工作的需求,为金刚石复合材料在光通信封装领域的产业化应用提供工程参考。
Abstract: With the large‑scale deployment of 1.6T and 3.2T high‑speed optical modules, the power consumption of optical chips, VCSEL arrays and TOSA/ROSA assemblies keeps rising. The local heat flux density has exceeded the heat dissipation limit of traditional heat‑sink materials such as copper, tungsten‑copper and AlN. Laser wavelength drift, bandwidth degradation and reduced long‑term reliability have become common industry pain points. Taking diamond/aluminum composite (diamond‑aluminum) as the core thermal diffusion material, this paper develops a complete thermal‑management solution for high‑speed optical transceiver modules and carries out engineering practices covering industry demand analysis, structural scheme design, theoretical thermal resistance calculation, mounting‑structure design, precision assembly process, comparative verification experiments and other procedures. The results show that replacing traditional copper heat sinks with diamond‑aluminum heat spreaders significantly reduces the junction temperature of optical chips, greatly narrows the temperature difference between devices and improves thermal‑cycle reliability. It can satisfy the requirements of next‑generation high‑speed optical modules for high‑density packaging, low thermal mismatch and stable high‑bandwidth operation, and provides engineering references for the industrial application of diamond‑matrix composites in optical‑communication packaging.
关键词:金刚石铝;金刚石复合材料;高速光模块;TOSA;热管理;热沉;热阻
Keywords: Diamond‑aluminum; Diamond‑matrix composite; High‑speed optical module; TOSA; Thermal management; Heat sink; Thermal resistance
一、行业需求分析
I. Industry Demand Analysis
在 AI 算力驱动下,数据中心光互连向单通道 100G、200G 演进,3.2T 光模块逐步进入送样与验证阶段。光模块内部集成 DFB 激光器、SOA、VCSEL 阵列、探测器、高速驱动芯片,器件封装空间高度受限,器件间距小、热串扰严重。
Driven by AI computing power, optical interconnections in data centers are evolving toward 100G and 200G per channel, and 3.2T optical modules are gradually entering the sampling and verification phase. Optical modules integrate DFB lasers, SOAs, VCSEL arrays, photodetectors and high‑speed driver chips. The packaging space for devices is highly constrained with small device spacing and severe thermal crosstalk.
- 热流密度需求:单颗光芯片功耗 5–12W,发光区面积仅 0.1–0.3 mm²,局部热流密度可达 300–600 W/cm²;传统纯铜热导率约 400 W/(m・K),WCu 热导率 200–260 W/(m・K),ALN 的热导率 180–220W/(m・K),热量扩散能力不足,热点集中,激光器结温超标,引发波长漂移、消光比劣化、误码率上升。
- 热膨胀匹配需求:GaAs、InP 光芯片 CTE 约 5.5–6.2×10⁻⁶/K,纯铜 CTE 高达 17×10⁻⁶/K,温度循环下焊层应力大、易脱焊、失效;金刚石 / 铝复合材料通过调控金刚石颗粒体积分数,可将 CTE 精准调控至 5–6×10⁻⁶/K,与光芯片、SiC 衬底高度匹配,降低封装热应力,提升长期可靠性。
- 封装与信号约束需求:光模块内部空间狭小,TOSA/ROSA 光路对装配平面度、台阶高度、端面垂直度要求极高;散热件不能引入额外寄生参数,避免干扰高速射频信号;同时要求材料可精密铣削、抛光、镀金,适配自动化封装产线。
- 国产化与长期可靠性需求:高端光模块热沉长期依赖进口,金刚石铝复合材料为国产替代路线;满足光模块规范的温度循环(-40℃~85℃)、高温老化、湿热测试要求,保证 20 年以上服役寿命。
- 轻量化需求:对比铜,无氧铜,钨铜,金刚石铝的密度 3.2g/cm³,分别相差 3、4.5 倍。
- 综上,行业迫切需要高热导率、CTE 可调、可精密加工、适配光封装工艺、轻量化方面的新型热扩散材料,金刚石 / 铝复合材料成为高速光模块热管理的优选方案。
- Heat‑flux density requirement: The power consumption of a single optical chip ranges from 5‑12 W, with the light‑emitting area merely 0.1‑0.3 mm², and the local heat‑flux density can reach 300‑600 W/cm². Traditional pure copper has a thermal conductivity of about 400 W/(m·K), W‑Cu 200‑260 W/(m·K), and AlN 180‑220 W/(m·K). They suffer from inadequate heat‑spreading capability, resulting in concentrated hot‑spots and excessive laser junction temperature, which triggers wavelength drift, extinction‑ratio degradation and higher bit‑error rate.
- Thermal‑expansion matching requirement: The CTE of GaAs and InP optical chips is approximately 5.5‑6.2×10⁻⁶/K, while pure copper has a high CTE of 17×10⁻⁶/K. Under thermal cycling, solder layers bear high stress and are prone to delamination and failure. By adjusting the volume fraction of diamond particles, diamond/aluminum composite can realize precisely‑tuned CTE of 5‑6×10⁻⁶/K. It matches well with optical chips and SiC substrates, reduces packaging thermal stress and improves long‑term reliability.
- Packaging and signal constraint requirement: Optical modules feature compact internal space. TOSA/ROSA optical paths impose extremely strict requirements on assembly flatness, step height and end‑face perpendicularity. Heat‑dissipating components shall not introduce extra parasitic parameters to avoid disturbing high‑speed RF signals. Meanwhile, the material is required to support precision milling, polishing and gold‑plating for compatibility with automated packaging production lines.
- Localization and long‑term reliability requirement: Heat sinks for high‑end optical modules have long depended on imports, and diamond‑aluminum composite provides a domestic‑substitution solution. It meets optical‑module specifications for thermal cycling (-40℃~85℃), high‑temperature aging and damp‑heat tests, ensuring a service life of more than 20 years.
- Light‑weighting requirement: Diamond‑aluminum has a density of 3.2 g/cm³, which is 3 times and 4.5 times lighter than copper, oxygen‑free copper and tungsten‑copper respectively.
- To sum up, the industry is in urgent demand for new thermal‑diffusion materials featuring high thermal conductivity, tunable CTE, precision machinability, compatibility with optical‑packaging processes and light weight. Diamond/aluminum composite has become the preferred solution for thermal management of high‑speed optical modules.
二、总体设计方案
II. Overall Design Scheme
2.1 材料选型
2.1 Material Selection
选用金刚石颗粒增强铝基复合材料(金刚石铝),金刚石体积分数 75%,实测热导率 800–850 W/(m・K),CTE 5.3×10⁻⁶/K,密度 3.2 g/cm³;表面做 Ti/Cr 过渡层 + 镍金电镀,满足可焊性、抗氧化、低界面接触电阻要求。 对比基准:纯铜热沉、WCu 热沉、AlN 陶瓷热沉。
Diamond‑particle‑reinforced aluminum‑matrix composite (diamond‑aluminum) is selected, with 75 vol% diamond. Its measured thermal conductivity is 800‑850 W/(m・K), CTE 5.3×10⁻⁶/K and density 3.2 g/cm³. A Ti/Cr transition layer plus Ni‑Au electroplating is applied on the surface to meet requirements for solderability, oxidation resistance and low interfacial contact resistance. Benchmarks for comparison: pure‑copper heat sink, W‑Cu heat sink, AlN ceramic heat sink.
2.2 散热链路设计(TOSA 封装架构)
2.2 Heat‑dissipation Chain Design (TOSA Packaging Architecture)
热传导链路:光芯片结区 → 金刚石铝均热片(热沉) → TIM 导热界面层 → 模块壳体 / 冷板 → 机柜风冷 / 液冷
方案定位:金刚石铝作为近端均热扩热沉,不直接做翅片,核心作用是把极小面积光芯片的集中热点快速摊开,降低扩散热阻,是整个散热链路的核心瓶颈优化环节。 结构分层:
1. 底层:金刚石铝均热基板(主热扩散层);
2. 中间层:焊层,光芯片 p-side 朝下贴装;
3. 上层:光路支架、透镜、隔离垫片;
4. 外侧:TIM 相变导热片连接至模块外壳。
Heat conduction chain: Optical‑chip junction zone → Diamond‑aluminum heat spreader (heat sink) → TIM thermal interface layer → Module housing / Cold plate → Cabinet air‑cooling / Liquid‑cooling.
Scheme positioning: Diamond‑aluminum acts as a near‑field heat‑spreading heat sink without integrated fins. Its core function is to rapidly spread concentrated hot‑spots from tiny‑area optical chips and reduce spreading thermal resistance, which is the key bottleneck‑optimization part of the whole heat‑dissipation chain.Structural layers:
- Bottom layer: Diamond‑aluminum heat‑spreading substrate (primary thermal‑diffusion layer);
- Middle layer: Solder layer, with optical chip mounted p‑side down;
- Upper layer: Optical‑path bracket, lens and isolation gasket;
- Outer side: Phase‑change TIM sheet connected to module housing
2.3 结构参数设计
2.3 Structural‑parameter Design
面向 3.2T 光模块 TOSA 组件,金刚石铝均热片尺寸:8 mm × 4 mm × 0.6 mm; 加工指标:平面度≤1 μm,表面粗糙度 Ra≤50 nm,端面倒角 R<1 μm,避免焊料爬至光学腔面污染光路; 局部预留定位台阶、定位销孔,保证光路同轴度,装配后光耦合损耗波动控制在 0.5 dB 以内。
For the TOSA assembly of 3.2T optical module, the dimension of diamond‑aluminum heat spreader is 8 mm × 4 mm × 0.6 mm.Processing specifications: Flatness ≤1 μm, surface roughness Ra ≤50 nm, end‑face chamfer radius R<1 μm, to prevent solder creeping onto optical cavity surfaces and contaminating optical paths. Locating steps and pin holes are reserved in local areas to guarantee optical‑path coaxiality, and the fluctuation of optical coupling loss after assembly is controlled within 0.5 dB.
2.4 仿真前置设计
2.4 Pre‑simulation Design
采用有限元热仿真(FEM),设置环境温度 25℃,光芯片功耗 10W,对比铜热沉与金刚石铝方案的温度场、温差、热流分布,初步判断结温降幅,再进入理论热阻计算与实物验证。
Finite‑element thermal simulation (FEM) is adopted. Ambient temperature is set to 25 ℃ and optical‑chip power consumption 10 W. Temperature field, temperature difference and heat‑flux distribution of copper‑heat‑sink scheme and diamond‑aluminum scheme are compared to preliminarily evaluate junction‑temperature reduction, before theoretical thermal‑resistance calculation and physical‑sample verification.
三、热阻计算过程
III. Thermal‑resistance Calculation Process
芯片温升 :当功耗 P=10W,原铜方案总热阻≈4.2 K/W,金刚石铝方案总热阻≈2.7 K/W;
铜方案温升≈42 K;金刚石铝方案温升≈27 K;
环境 25℃时,铜方案结温≈67℃;金刚石铝方案结温≈52℃。
Chip temperature rise: At power consumption P=10 W, the total thermal resistance of the original copper scheme is approx. 4.2 K/W, while that of diamond‑aluminum scheme is approx. 2.7 K/W.
Temperature rise of copper scheme ≈42 K; temperature rise of diamond‑aluminum scheme ≈27 K.
At ambient temperature of 25 ℃, the junction temperature of copper scheme is approx. 67 ℃, and that of diamond‑aluminum scheme approx. 52 ℃.
四、安装方案设计
IV. Mounting‑scheme Design
4.1 安装定位基准
4.1 Mounting and Positioning Datum
采用定位销 + 台阶限位的复合定位方案,金刚石铝热沉预留 2 个 Φ0.8 mm 定位销孔,与 TOSA 陶瓷基座销钉配合,保证热沉与光芯片、透镜的同轴度,避免装配偏移带来耦合损耗变化。 安装基准面:热沉下表面为散热基准面,上表面为芯片贴装基准面,两面平行度≤0.8 μm。
A composite positioning scheme combining locating pins and step limits is adopted. Two Φ0.8 mm locating pin holes are reserved on diamond‑aluminum heat sink to cooperate with pins on TOSA ceramic base, ensuring coaxiality among heat sink, optical chip and lens and preventing coupling‑loss variation caused by assembly offset.Mounting datum planes: The lower surface of heat sink serves as heat‑dissipation datum plane, and the upper surface as chip‑mounting datum plane. The parallelism between the two planes is ≤0.8 μm.
4.2 安装压紧与应力控制
4.2 Mounting Compression and Stress Control
光芯片属于脆性光电器件,严禁刚性硬压。采用弹性压紧工装:真空吸附 + 低压力弹簧压头,贴装、回流焊阶段压力控制在 0.3–0.5 N,防止芯片碎裂、外延层损伤;焊后工装释放,无持续机械应力。
Optical chips are brittle optoelectronic devices and rigid hard compression is strictly prohibited. Elastic compression tooling consisting of vacuum suction and low‑force spring indenter is applied. The pressure is controlled at 0.3‑0.5 N during mounting and reflow soldering to avoid chip cracking and epitaxial‑layer damage. The tooling is released after soldering without sustained mechanical stress.
4.3 散热对接方案
4.3 Heat‑dissipation Interface Scheme
金刚石铝底部与模块壳体之间采用相变导热材料(PCM TIM),厚度 25 μm,熔融温度 45℃,低温下固态定型,高温熔化填充微间隙,界面热阻低;不使用高粘度导热硅脂,避免长期溢胶污染光路。
Phase‑change thermal‑interface material (PCM TIM) with 25 μm thickness and 45 ℃ melting temperature is adopted between the bottom of diamond‑aluminum component and module housing. It remains solid at low temperature and melts to fill micro‑gaps at high temperature for low interfacial thermal resistance. High‑viscosity thermal grease is avoided to prevent long‑term glue overflow from contaminating optical paths.
4.4 防污染与光路隔离
4.4 Anti‑contamination and Optical‑path Isolation
热沉靠近光学腔一侧做限位挡边,挡边高出芯片表面 8 μm,形成焊料阻挡坝,回流焊时焊料被限制在贴装区域,杜绝焊料爬边污染光学端面,是光模块封装特有的安装约束设计。
A limiting baffle is arranged on the heat sink beside the optical‑cavity side. The baffle is 8 μm higher than the chip surface to form a solder dam. Solder is confined within the mounting area during reflow soldering so as to eliminate solder creeping and optical‑end‑face contamination. This is a unique mounting‑constraint design for optical‑module packaging.
五、装配工艺(精密封装流程)
V. Assembly Process (Precision Packaging Flow)
整套工艺面向光模块 TO/TOSA 自动化封装线,分为来料处理、表面活化、贴装、回流焊、清洗、耦合、终检 7 个工序:
1. 来料检验与预处理 金刚石铝热沉来料抽检:热导率、平面度、粗糙度、镀金层附着力;等离子清洗(Ar 等离子),去除表面有机污染物,提升焊层浸润性;
2. 焊料预制 在金刚石铝芯片贴装区域,预制 5 μm 厚焊片,对位贴合;
3. 光芯片贴装(P-down) 真空共晶贴片机,视觉定位,将 InP 光芯片 p 面向下精准贴于焊片上,定位精度 ±3 μm;
4. 等离子清洗 焊后二次等离子清洗,去除焊剂残留、微小金属飞溅物,防止长期电迁移;
5. 光学耦合装配 装配透镜、隔离器、光纤适配器,在线监测光功率、消光比,完成耦合固化;
6. 热界面装配与壳体封装 在金刚石铝底部贴装相变 TIM 片,装入模块外壳,锁紧固定螺钉,螺钉扭矩标准化 0.08 N・m,扭矩过大易挤压变形、过小界面热阻上升。
工艺管控要点:全程洁净车间 Class 1000,静电防护,热沉禁止徒手接触光学侧边贴装区。
The whole process targets automated TO/TOSA packaging lines for optical modules, including seven working procedures: incoming‑material treatment, surface activation, mounting, reflow soldering, cleaning, optical coupling and final inspection.
- Incoming‑material inspection and pre‑treatment: Sampling inspection for incoming diamond‑aluminum heat sinks covers thermal conductivity, flatness, roughness and gold‑plating‑layer adhesion. Ar‑plasma cleaning removes surface organic contaminants and improves solder‑layer wettability.
- Solder preforming: A 5‑μm‑thick solder preform is placed and aligned on the chip‑mounting area of diamond‑aluminum component.
- Optical‑chip mounting (P‑down): A vacuum eutectic bonder with visual‑alignment system precisely mounts InP optical chip p‑side down onto the solder preform with positioning accuracy of ±3 μm.
- Plasma cleaning: Secondary plasma cleaning after soldering removes flux residues and tiny metal spatter to prevent long‑term electromigration.
- Optical coupling assembly: Lenses, isolators and fiber adapters are assembled. Optical power and extinction ratio are monitored on‑line to complete coupling and curing.
- Thermal‑interface assembly and housing packaging: Phase‑change TIM sheet is attached to the bottom of diamond‑aluminum part, then assembled into module housing. Fixing screws are tightened with standardized torque of 0.08 N·m. Excessive torque may cause compressive deformation while insufficient torque leads to higher interfacial thermal resistance.Key process‑control points: The whole workflow is carried out in Class‑1000 clean‑room with ESD protection. Manual bare‑hand contact with optical‑side mounting area of heat sink is forbidden.
六、实验验证与效果分析
VI. Experimental Verification and Performance Analysis
6.1 实验条件
6.1 Experimental Conditions
被测对象:3.2T 光模块 TOSA 组件; 对比样 A:传统纯铜热沉;对比样 B:金刚石铝热沉; 测试环境:恒温箱 25℃,模块上电,单通道持续 10W 热耗; 测试设备:红外显微热成像仪、高速光示波器、光谱分析仪、温度循环试验箱。
Tested object: TOSA assembly of 3.2T optical module.Comparative sample A: Traditional pure‑copper heat sink; Comparative sample B: Diamond‑aluminum heat sink.Test environment: Temperature chamber set at 25 ℃, module powered‑on with continuous single‑channel power dissipation of 10 W.Test equipment: Infrared micro‑thermal imager, high‑speed optical oscilloscope, optical spectrum analyzer, thermal‑cycling test chamber.
6.2 静态热测试结果
6.2 Static Thermal Test Results
纯铜方案:芯片最高结温 64.5℃,芯片表面温差 9.2 K;
金刚石铝方案:芯片最高结温 49.1℃,芯片表面温差 2.8 K; 结温降幅约 15.4℃,芯片面内均匀性显著提升,热串扰被抑制。
Pure‑copper scheme: Maximum chip junction temperature 64.5 ℃, chip surface temperature difference 9.2 K.
Diamond‑aluminum scheme: Maximum chip junction temperature 49.1 ℃, chip surface temperature difference 2.8 K. The junction‑temperature reduction reaches about 15.4 ℃. The in‑plane temperature uniformity of chip is greatly improved and thermal crosstalk is suppressed.
6.3 光学性能测试
6.3 Optical‑performance Test
在相同驱动条件下: 铜热沉方案:温度升高后激光器波长漂移 0.72 nm,消光比下降 1.2 dB; 金刚石铝方案:波长漂移 0.23 nm,消光比衰减<0.3 dB; 窗口明显拓宽,高温下带宽稳定性显著改善。
Under identical driving conditions:‑ Copper‑heat‑sink scheme: Laser wavelength drift of 0.72 nm and extinction‑ratio degradation of 1.2 dB with temperature rise.‑ Diamond‑aluminum scheme: Wavelength drift of 0.23 nm and extinction‑ratio degradation <0.3 dB.The operating window is obviously broadened and bandwidth stability at high temperature is remarkably enhanced.
6.4 可靠性验证(温度循环)
6.4 Reliability Verification (Thermal Cycling)
循环条件:-50℃ ↔ 150℃,15 min 一个循环,1000 次;
铜热沉样品:3 只样品中 1 只出现焊层微裂纹,光功率衰减>10%;
金刚石铝样品:5 只样品光功率、光谱、耦合损耗无明显劣化,无焊层失效,低 CTE 匹配优势充分体现。
Cycling condition: ‑50 ℃ ↔ 150 ℃, 15 min per cycle, 1000 cycles in total.
Copper‑heat‑sink samples: Among 3 samples, one develops micro‑cracks in solder layer with optical‑power attenuation over 10%.‑
Diamond‑aluminum samples: No obvious degradation in optical power, optical spectrum or coupling loss among 5 samples; no solder‑layer failure occurs. The advantages of low‑CTE matching are fully demonstrated.
6.5 短板说明
6.5 Limitation Description
金刚石铝材料成本高于普通铜;硬脆特性决定不能做大切削加工;烧结工艺对界面结合控制要求高,一旦界面碳化物层不良,热导率会大幅衰减。
Diamond-aluminum composite has a higher cost than ordinary copper. Due to its hard and brittle property, it cannot undergo heavy cutting machining. The sintering process requires rigorous control of interfacial bonding. Defective interfacial carbide layers will result in a significant reduction in thermal conductivity.
七、结论与工程展望
VII. Conclusions and Engineering Outlook
本文完成金刚石 / 铝复合材料在高速光模块 TOSA 组件的完整工程化应用实践,从行业热管理痛点出发,完成材料选型、热链路设计、热阻理论计算、定位安装结构、精密共晶装配、多维度验证实验。 金刚石铝凭借高热导率、可调控热膨胀系数两大核心优势,相比传统铜热沉,可有效降低光芯片结温、减小器件温差、抑制激光器波长漂移,同时大幅提升温度循环下封装可靠性,适配 1.6T、3.2T 及下一代更高速率光模块的封装需求。
This paper completes full‑scale engineering application practice of diamond/aluminum composite in TOSA assemblies of high‑speed optical modules. Starting from industry thermal‑management pain points, it covers material selection, heat‑chain design, theoretical thermal‑resistance calculation, positioning‑mounting structure, precision eutectic assembly and multi‑dimensional verification experiments. Benefiting from its two core merits of high thermal conductivity and tunable CTE, diamond‑aluminum can effectively reduce optical‑chip junction temperature, narrow device temperature difference and restrain laser wavelength drift compared with traditional copper heat sinks. Meanwhile, it greatly improves packaging reliability under thermal cycling and meets packaging requirements for 1.6T, 3.2T and future higher‑rate optical modules.